Substrate Suitability, Assessment and Preparation
Substrate Suitability
Bauder LiquiTEC is suitable for both New Build and Refurbishment applications as a Cold or Inverted Roof design. It can be applied directly onto concrete decks and can also be applied to most existing waterproofing membranes as an overlay membrane. Timber decks will require the prior application of a carrier membrane to bridge panel joints and take up any movement between them. Refer to the specific project specification for further details. It is essential that a proper assessment of the substrate is carried out in all cases and that adhesion tests and thorough preparation are undertaken before commencement
Substrate assessment
- Structural assessment
- Ensure that the structure is designed to withstand the proposed loadings.
- Any existing known structural defects must be rectified prior to overlay.
- Concrete structures should be designed in accordance with BS8110/CP110.
- Timber / plywood decks must be constructed from minimum 15mm exterior grade plywood, with joists at max 450mm centres and minimum 18mm for up to 600mm centres. Deck to be mechanically fixed with countersunk fixings at 100mm centres along all joists and noggins.
- General substrate assessment
- Assess the stability of the underlying substrate prior to the commencement of work.
- Surfaces to be coated including existing repair materials must be firmly fixed.
- Dimensional stability
- All factors which may affect the subsequent performance of the roof, e.g. saturated insulation, failed structural elements etc. must be removed, repaired or replaced.
- Falls
A design fall of minimum 1:40 is recommended in order to ensure a constructed fall of minimum 1:80 is achieved. However, the Bauder LiquiTEC system is suitable for application to zero pitch roofs, but it is essential that any areas of backfalls or deflection are levelled prior to installing the system.
- Surface moisture
The surface must be dry prior to overlay with Bauder LiquiTEC.
Theoretical check:
- The surface temperature must be higher than the dew point (this can be calculated – see page 16).
Practical checks
- If it looks wet, feels wet, appears wet – it is unlikely to be dry!
- Apply a tissue to the surface and ensure dry when removed.
Moisture content (cementitious materials)
Prior to overlay with Bauder LiquiTEC systems, the equilibrium moisture content of the substrate must not exceed 6% by weight or 75% RH.
Ensure that moisture will not come into contact with the underside of the coating due to structural conditions. Bauder LiquiTEC is not a DPM.
Measured checks:
- Carry out RH test in accordance with British Standard using a suitable hygrometer (eg. GE Protimeter MMS). Please note this is a non-destructive method but lacks accuracy.
- Carry out equilibrium moisture test with CM tester. This is a destructive method to check the actual moisture content of the sample.
Note: Both methods give a result for the sample only and not the deck as a whole.
Practical advice
Lower risk scenarios
- Refurbishment (hydration complete)
- If the surface is closed with few voids e.g. power floated
- If the substrate is white / light grey
- If the substrate looks impermeable
- If there is no buried membrane or permanent formwork
- If the substrate has previously been waterproofed
- If the cementitious material is polymer modified
- If the area has good falls
- If the area is under cover
Higher risk scenarios
- New build (hydration incomplete – green concrete)
- Sand and cement screeds
- Anything brown
- If the surface is open with voids
- If the substrate looks porous / contains porous aggregates (lytag)
- If there is a buried membrane* or permanent formwork
- If the substrate has never previously been waterproofed
- If the area has poor falls
- If the area is exposed
Practical checks
- Dry core and break the sample or simply remove a sample (hammer and chisel) and observe apparent moisture levels at the surface and deeper within the build up. If anything looks damp / wet do not proceed.
- Use adhesion testing / observation of primer coat.
- Prepare and prime an area and look for:
- Blisters
- Blooming / milkiness
- Adhesion: If a risk is perceived set a limit for adhesion higher than standard (e.g. 2.0N/mm²)
Minimising the risk
- Prime the higher risk areas first, but leave as long as possible before overlaying. If the primer shows any of the problems listed above, the substrate is not sufficiently dry.
Specific advice for new concrete
- Consult the engineer / concrete supplier for details of the mix and the estimated hydration times.
- Allow minimum 28 days.
Hardness
Substrates should achieve a minimum hardness of 25N/mm².
Measured checks
- Carry out compressive strength tests with a “Schmidt” hammer.
Practical checks
- With particular regard to cementitious substrates, if the surface is not friable, cannot be eroded with the heel of a shoe, does not feel soft or crumbly, the compressive strength is likely to be higher than 25N/mm².
- If the existing substrate is trafficked and has been subjected to point loadings without indentation, then it is likely to be suitable for overlay with a trafficable system.
Substrate Preparation
Basic requirements
- The substrate must be clean, dry and free from dust, laitance, grease, oil and any other contaminants.
- Where there are existing coatings, paints or sealers fully remove (or carry out on site adhesion tests to determine suitability for overlay).
- For timber / plywood decks, a suitable carrier membrane is to be applied prior to applying the Bauder LiquiTEC system. Refer to specific project specification for more details.
Initial Cleaning Equipment / Methods
Pressure Washer (2,000 psi)
- Washing down / organic growth removal.
Typical Preparation Equipment
- Brushing – use of a stiff brush for removal of dirt and dust.
- Scarifier - for de-chipping/preparation of certain cementitious materials etc.
- Open shot blasting - for coating removal/cementitious materials/asphalt.
- Hand grinder (diamond / carbide) – for detail preparation.
- Sanding – for detail preparation/metals/plastic/certain single ply membranes.
Substrate Preparation & Priming Schedule
| Substrate | Preparation Notes | Main area | Details |
|---|---|---|---|
| Asphalt | 1/8 | Bauder LiquiPRIME 1 | Bauder LiquiPRIME 1 |
| Polymer modified asphalt | 1/8 | Bauder LiquiPRIME 1 | Bauder LiquiPRIME 1 |
| Oxidised bitumen membrane | 2/9 | Bauder LiquiPRIME 1 to exposed bitumen only | Bauder LiquiPRIME 1 to exposed bitumen only |
| SBS modified bitumen membrane | 2/9 | Bauder LiquiPRIME 1 to exposed bitumen only | Bauder LiquiPRIME 1 to exposed bitumen only |
| APP modified bitumen membrane | 2/9 | Bauder LiquiPRIME 1 to exposed bitumen only | Bauder LiquiPRIME 1 to exposed bitumen only |
| Bitumen | 2 | Bauder LiquiPRIME 1 | Bauder LiquiPRIME 1 |
| Concrete / Screed / Brickwork | 1/5 | Bauder LiquiPRIME 2 | Bauder LiquiPRIME 2 |
| New Concrete / Porous concrete | 1/5 | Cryl Primer 287 | Cryl Primer 287 |
| Concrete with 6-10% equilibrium moisture content | 1 | Seek Bauder advice | Seek Bauder advice |
| Lightweight concrete / render | 1 | Seek Bauder advice | Seek Bauder advice |
| Polymer modified concrete | 1/5 | Bauder LiquiPRIME 2 | Bauder LiquiPRIME 2 |
| Blockwork (porous) | 1/5 | Bauder LiquiPRIME 2 at 0.6Kg/m² with maximum catalyst + 1% Liquid Thixo | Bauder LiquiPRIME 2 at 0.6Kg/m² with maximum catalyst + 1% Liquid Thixo |
Single ply membranes:
| Substrate | Preparation Notes | Main Area | Details |
|---|---|---|---|
| CPE | 3/7 | No primer required | No primer required |
| EVA | 2/7 | No primer required | No primer required |
| PIB | 2/7 | No primer required | No primer required |
| PVC-P, nB | 3/7 | No primer required | No primer required |
| Other single-ply membranes | Subject to testing | ||
Preparation notes
| 1 | Scarify, grind or lightly bead blast. |
| 2 | Scrape and sweep away contamination and clean by power washing (with or without approved detergent) as required. |
| 3 | Rub down thoroughly with Bauder PMMA Cleaner and abrade / grind metals and hard plastics to achieve a roughened surface. (Steel must be ground or blasted to bright metal – where all rust cannot be practically removed, use “Hammerite No.1 Rustbeater” prior to the application of Bauder LiquiTEC products). |
| 4 | Lightly abrade and carry out an adhesion test as described in this manual. |
| 5 | The equilibrium moisture content of cementitious materials must not exceed 6% or 75% RH. Where moisture levels are in excess of these values seek advice from Bauder regarding possible use of Pox R106. |
| 6 | Subject to testing of insitu material and approval by Bauder Technical Team. |
| 7 | Where large areas are to be treated, test areas to be carried out to ensure ruckling does not occur. |
| 8 | Blisters and high spots should be cut away using a grinder. Do not heat and trowel. |
| 9 | Loose areas and blisters to be cut away. |
Where there are any doubts as to adhesion, preparation or substrate stability carry out adhesion tests as described in this manual.
For other substrates, consult the Bauder Technical Department on 01473 257671 for required preparation methods and priming.
The importance of Adhesion
After applying a test area of Bauder LiquiDEK (and recommended primer if required), cut a circular hole through the Bauder coating and upper layers of the substrate with a hole saw. Adhere 50mm dolly to the surface of the LiquiDEK within the cut area and allow adhesive to cure.
Carry out adhesion test with calibrated hydraulic test rig.
The LiquiTEC system should achieve a minimum bond to the substrate of:
- Cementitious materials / metals / plastics / hard substrates: 1.50N/mm²
- Asphalt and other substrates: 0.80N/mm²
- Unbonded / loose laid substrates where pull off tests not possible (membranes): Peel strength adhesion 30N/50mm
Measured checks
- Carry out pull off tests using minimum 50mm dollies and carefully assess results.
- Carry out DIN EN 12316 peel strength adhesion tests.
Practical checks
- Carry out pull off tests using minimum 50mm dollies and calibrated hydraulic test rig and carefully assess results (as detailed above).
- Carry out on site peel tests.
Peel test method
Carry out adhesion tests as illustrated below:
- Prepare substrate and apply resins.
Waiting times before peeling
| Substrate | Waiting Time |
|---|---|
| Synthetic single ply membranes | min. 3 hours |
| Coated materials e.g. metals | min. 3 hours |
| Cementitious materials | min. 3 hours |
| Bituminous materials | min. 3 hours and ideally after 72 hours due to lower initial adhesion |
- Peel method: Hold the exposed fleece and pull slowly at 90 degrees to the substrate.
150mm x 150mm Bauder LiquiDEK (with Bauder 110g reinforcement fleece)
Prepared / primed sample area (300mm x 300mm)
50mm exposed Bauder 110g reinforcement fleece tab
Assessment
| Mode of failure | Assessment |
|---|---|
| Cannot be removed | Satisfactory adhesion |
| Fleece tears | Satisfactory adhesion |
| Interlayer delamination of LiquiDEK membrane | Satisfactory adhesion |
| LiquiDEK membrane difficult to remove and removes top layer of homogenous substrate (not coating) | Satisfactory adhesion |
| LiquiDEK membrane easy to remove with little or no LiquiDEK material left on substrate, or substrate on LiquiDEK membrane | Poor adhesion – re-test using different preparation / primer / combinations and leave for a minimum of 72 hours |
| LiquiDEK membrane easy to remove and removes coating (paint etc.) from coated substrate | Poor adhesion – remove coating from substrate and re-test |