Trouble Shooting

Operation / productProblemCausesSolution
Primer

Bauder LiquiPRIME 1 & 2
Primer does not cure
(or remains wet or very sticky)
Too Little or no Catalyst
Applied too thinly
Incorrectly mixed
Poor substrate preparation
Porous substrate
Reaction with substrate
Remove the primer
Clean with Bauder PMMA Cleaner
Test to ensure a reaction has not occurred

Apply new primer with correct catalyst (upper limit) at minimum consumption or above.

Defects in the primer
(incomplete film/tacky surface)
Applied too thinly
Applied by squeegee and not working in both directions
Too little or no catalyst
Incorrectly mixed
Poor substrate preparation
Porous substrate
Test and if suitable: Reapply primer to defective areas immediately wet in wet using maximum catalyst and minimum consumption of above.

Primer lifting at the edges/primer shattersPrimer applied too thicklyRemove all loose/shattered sections
Reapply primer to defective areas.

Lumps form on the primed surfacePrimer applied after the end of pot lifeRemove lumps with a trowel or by sanding down.
Reapply primer to defective areas.
Paste

Bauder LiquiPASTE
Paste does not cureToo little or no catalyst
Incorrectly mixed
Remove the paste.
Clean with Bauder PMMA Cleaner and allow to evaporate.
Reapply paste.
Waterproofing

Bauder LiquiDEK
Bauder LiquiDETAIL
Waterproofing does not cure/delaminates from substrateToo little or no catalyst
Incorrectly mixed
First layer of resin applied under the fleece is too thin.
Completely remove the waterproofing.
Clean the area with Bauder PMMA Cleaner and allow to evaporate.
Abrade the substrate.
Re-apply primer if necessary.
Re-apply waterproofing.

Blistering in the waterproofingAir pockets – the fleece is not embedded correctly
First layer of resin applied under the fleece is too thin
Incorrectly mixed
Defects in the primer
Cut open the blisters and remove.
Remove material that has failed to cure fully.
Clean the area with Bauder PMMA Cleaner.
Mechanically roughen the substrate.
Reapply primer if necessary.
Reapply waterproofing.

Waterproofing has cured but is tackyTemperatures too high or too low
No/low air movement
Clean the area with Bauder PMMA Cleaner and allow to evaporate.
If required apply additional layer of resin/finish – subject to testing.